ASTM B409 covers UNS N08120, UNS N08890, UNS N08800, UNS N08810, and UNS N08811 in the form of rolled plate, sheet, and strip. Alloy UNS N08800 is normally employed in service temperatures up to and including 1100°F (593°C). Alloys UNS N08120, UNS N08810, UNS N08811, and UNS N08890 are normally employed in service temperatures above 1100°F (593°C) where resistance to creep and rupture is required, and they are annealed to develop controlled grain size for optimum properties in this temperature range.

ASTM B409 Plate, Sheet, and Strip Specifications
- Applicable Product Forms: Rolled plates, sheets, and strips (Plate, Sheet & Strip).
- Applicable Grades: UNS N08120 (Haynes HR-120), UNS N08890, UNS N08800 (Alloy 800), UNS N08810 (Alloy 800H), UNS N08811 (Alloy 800HT).
- Temperature Applications: N08800 is typically used at temperatures of 593°C and below; N08120, N08810, N08811, and N08890 are used in applications above 593°C that require high creep and endurance strength and must be annealed to achieve controlled grain size.
- Chemical Composition: The elemental composition of each grade must comply with the ranges specified by UNS. The supplier must provide a Melt Test Report (MTR), and the deviations in the finished product analysis must comply with the product analysis tolerances in Table 2 of the standard.
- Heat Treatment Condition: Delivered in a solution-annealed condition; for example, N08120 requires rapid cooling (water quenching or rapid air cooling) at 1175–1225°C to prevent sensitization; The heat treatment curve must be available for reference in the MTR.
- Mechanical Properties: Minimum tensile strength, yield strength, and elongation values are specified based on the product form and grade. For example, for N08120 sheet, the tensile strength is ≥690 MPa, the yield strength is ≥310 MPa, and the elongation is ≥30%; for N08800, the tensile strength is ≥520
General Requirements
Material furnished under this specification shall conform to the applicable requirements of Specification B906 unless otherwise provided herein
Chemical Composition
| Element | Alloy N08120 | Alloy N08890 | Alloy N08800 | Alloy N08810 | Alloy N08811 |
|---|---|---|---|---|---|
| Nickel | 35.0-39.0 | 40.0-45.0 | 30.0-35.0 | 30.0-35.0 | 30.0-35.0 |
| Chromium | 23.0-27.0 | 23.0-28.5 | 19.0-23.0 | 19.0-23.0 | 19.0-23.0 |
| Iron | remainder (B) | remainder | ≥39.5 (B) | ≥39.5 (B) | ≥39.5 (B) |
| Manganese | ≤1.5 | ≤1.5 | ≤1.5 | ≤1.5 | ≤1.5 |
| Carbon | 0.02-0.10 | 0.06-0.14 | ≤0.10 | 0.05-0.10 | 0.06-0.10 |
| Copper | ≤0.50 | ≤0.75 | ≤0.75 | ≤0.75 | ≤0.75 |
| Silicon | ≤1.0 | 1.0-2.0 | ≤1.0 | ≤1.0 | ≤1.0 |
| Sulfur | ≤0.03 | ≤0.015 | ≤0.015 | ≤0.015 | ≤0.015 |
| Aluminum | ≤0.4 | 0.05-0.60 | 0.15-0.60 | 0.15-0.60 | 0.25-0.60 (C) |
| Titanium | ≤0.2 | 0.15-0.60 | 0.15-0.60 | 0.15-0.60 | 0.25-0.60 (C) |
| Molybdenum | ≤2.5 | 1.0-2.0 | … | … | … |
| Niobium (D) | 0.4-0.9 | 0.2-1.0 | … | … | … |
| Tantalum | … | 0.10-0.60 | … | … | … |
| Phosphorus | ≤0.04 | … | ≤0.045 | ≤0.045 | ≤0.045 |
| Tungsten | ≤2.5 | … | … | … | … |
| Cobalt | ≤3.0 | … | … | … | … |
| Nitrogen | 0.15-0.30 | … | … | … | … |
| Boron | ≤0.01 | … | … | … | … |
(B) Iron shall be determined arithmetically by difference.
(C) Alloy N08811:Al +Ti=0.85- 1.20
(D) Columbium and Niobium are interchangeable names for the same element and both names are acceptable for use in B02.07 specifications
Mechanical Properties
| Alloy | Condition | Tensile Strength, min, psi (MPa) | Yield Strength (B) (0.2 % offset), min, psi (MPa) | Elongation in 2 in. or 50 mm (or 4D), min, % |
|---|---|---|---|---|
| Hot-Rolled Plate | ||||
| UNS N08120 | Annealed | 90000 (621) | 40000 (276) | 30 |
| UNS N08800 | Annealed | 75000 (520) | 30000 (205) | 30 |
| UNS N08800 | As-rolledCD | 80000 (550) | 35000 (240) | 25 |
| UNS N08810 | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08811 | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08890 | Annealed | 75000 (520) | 30000 (205) | 35 |
| Hot-Rolled Sheet | ||||
| UNS N08120 | Annealed | 90000 (621) | 40000 (276) | 30 |
| UNS N08800 | Annealed | 75000 (520) | 30000 (205) | 30 |
| UNS N08810D | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08811D | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08890 | Annealed | 75000 (520) | 30000 (205) | 35 |
| Cold-Rolled Sheet | ||||
| UNS N08120 | Annealed | 90000 (621) | 40000 (276) | 30 |
| UNS N08800 | Annealed | 75000 (520) | 30000 (205) | 30 |
| UNS N08810 (E) | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08811 (E) | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08890 | Annealed | 75000 (520) | 30000 (205) | 35 |
| Cold-Rolled Strip | ||||
| UNS N08120 | Annealed | 90000 (621) | 40000 (276) | 30 |
| UNS N08800 | Annealed | 75000 (520) | 30000 (205) | 30 (F) |
| UNS N08810(E) | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08811(E) | Annealed | 65000 (450) | 25000 (170) | 30 |
| UNS N08890 | Annealed | 75000 (520) | 30000 (205) | 35 |
B Yield strength requirements do not apply to material under 0.020 in. (0.51 mm) in thickness
C As-rolled plate may be given a stress-relieving heat treatment subsequent to final rolling.
D As roled plate speciied “suitable for hotforming shallbe furished rom heats of known good hot malleabity characteristics(see X1.1.1.2). Tne purchaser must specify Alloy UNS No8800 or UNS No8810. There are no applicable tensile or hardness requirements for such material.
E Available only in thicknesses 0.115 in. (2.92 mm) and over.
F Not applicable for thickness under 0.010 in. (0.25 mm).
Materials and Manufacture
Heat Treatment-The minimum temperature of the finalheat treatment for each alloy shall be as follows:
- UNS NO8120 2150 °F (1177 °C);
- UNS NO8810-2050 °F (1121 °C);
- UNS NO8811 and UNS NO8890-2100 °F (1149 °C).
Grain Size
Annealed Alloys UNS N08120, UNS N08810, UNS N08811, and UNS N08890 shall conform to an average grain size of ASTM No. 5 or coarser.
Dimensions and Permissible Variations
Thickness and Weight:
Plate-For plate up to 2 in. (50.8 mm), incl, in thickness, the permissible variation under the specified thick-ness and permissible excess in overweight shall not exceed the amounts prescribed in Table A3.1 in Specification B906.
For use with Table A3.1 in Specification B906, plate shall be assumed to weigh 0.287 lb/in.3 (7.944 g/cm3).
Plate-For plate over 2 in. (50.8 mm) in thickness, the permissible variations over the specified thickness shall not exceed the amounts prescribed in Table A3.2 in Specification B906.
Sheet and Strip – The permissible variations in thick-ness of sheet and strip shall be as prescribed in Table A3.3 in Specification B906. The thickness of sheet and strip shall be measured with the micrometer spindle 3/8 in. (9.5 mm) or more from either edge for material 1 in. (25.4 mm) or over in width and at any place on strip under 1 in. in width.
Width or Diameter
Plate – The permissible variations in width of rectangular plates and diameter of circular plates shall be as prescribed in Table A3.4 and Table A3.5 in Specification B906.
Sheet and Strip – The permissible variations in width for sheet and strip shall be as prescribed in Table A3.6 in Specification B906.
Length:
Sheet and strip of all sizes may be ordered to cut lengths, in which case a variation of 1/8 in. (3.18 mm) over thespecified length shall be permitted.
Permissible variations in length of rectangular plate shall be as prescribed in Table A3.7 in Specification B906.
Straightness:
The edgewise curvature (depth of chord) of flat sheet,strip, and plate shall not exceed 0.05 in. multiplied by the length in feet (0.04 mm multiplied by the length in centimetres).
Straightness for coiled strip material is subject to agreement between the manufacturer and the purchaser.
Edges
When finished edges of strip are specified in the contract or order, the following descriptions shall apply:
Square-edge strip shall be supplied with finished edges, with sharp, square corners, without bevel or rounding.
Round-edge strip shall be supplied with finished edges, semicircular in form, the diameter of the circle forming the edge being equal to the strip thickness.
When no description of any required form of strip edge is given, it shall be understood that edges such as those resulting from slitting or shearing will be acceptable.
Sheet shall have sheared or slit edges.
Plate shall have sheared or cut (machined, abrasive-cut, powder-cut, or inert arc-cut) edges, as specified.
Squareness (Sheet):
For sheets of all thicknesses, the angle between adjacent sides shall be 90 + 0.15° (1/16 in. in 24 in.) (1.59 mmin 610 mm).
Flatness:
There shall be no flatness requirements for “deep-drawing quality” and “spinning quality” sheet and strip (see X1.1.3).
Standard flatness tolerances for plate shall conform to the requirements of Table 5, “Specially-flattened” plate when so specified, shall have permissible variations in flatness as agreed upon between the manufacturer and the purchaser.
Test Methods
The chemical composition, mechanical, and otherproperties of the material as enumerated in this specificationshall be determined, in case of disagreement, in accordancewith the methods in Specification B906.
The measurement of average grain size may be carriedout by the planimetric method, the comparison method, or theintercept method described in Specification B906. In case ofdispute, the “referee” method for determining average grainsize shall be the planimetric method.
For purposes of determining compliance with thespecified limits for requirements of the properties listed inSpecification B409, an observed value or a calculated valueshall be rounded in accordance with the rounding methods inSpecification B906.
Product Marking
Each bundle or shipping container shall be marked with the name of the material; condition (temper); this specification number; the size; gross, tare, and net weight; consignor and consignee address; contract or order number; or such other information as may be defined in the contract or order.
Conditions(Tempers)And Finishes
Plate, Hot Rolled
Annealed – Soft with an oxide surface,and suit-able for heavy cold forming.Available with a descaled surface,when so specified.
As-Rolled-With an oxide surface.Available witha descaled surface,when so specified.Suitable for flat work,mild forming,or tube sheets.When intended for tube sheets,specify that plates are to be specially flattened. When intendedfor hot forming,this should be indicated on the purchase orderso that the manufacturer may select appropriate material.
Plate, Cold Rolled
Annealed – Soft with an oxide surface;available with a descaled surface when so specified.
Sheet, Hot-Rolled Annealed and Pickled
Soft with a pickled matte finish.Properties similar to annealed condition but with broader thickness tolerances. Not suggested for applications where the finish of a cold-rolled sheet is considered essential, or for deep drawing, or spinning.
Sheet and Strip, Cold-Rolled
Annealed-Soft with a descaled or bright annealed finish.
Deep-Drawing or Spinning Quality-Similar to Annealed condition, except furnished to controlled hardness and grain size and lightly leveled.
ASTM B409 Plate, Sheet, and Strip Sizes
- Cold-rolled sheet: Thicknesses of 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.5 mm, 2.0 mm, 2.5 mm, 3.0 mm, and 4.0 mm; standard widths of 1,000 mm, 1,219 mm, and 1,500 mm.
- Hot-Rolled Medium Plates: Thicknesses 5 mm, 6 mm, 8 mm, 10 mm, 12 mm, 14 mm, 16 mm, 18 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm.
- Thick Plate/Extra-Thick Plate: 55 mm, 60 mm, 65 mm, 70 mm, 80 mm, 90 mm, 100 mm, 120 mm, 150 mm; customizable up to 200 mm; widths ranging from 2,000 to 3,000 mm.
- Strips/Coils: Precision foil 0.02 mm–0.10 mm; narrow strips/wide strips 0.15 mm–3.0 mm, with widths ranging from 5 mm to 1,500 mm; slitting, lamination, and precision shearing available.
UNS Numbers and Commercial Designations
- UNS N08800: Corresponds to Incoloy 800 or Alloy 800
- UNS N08810: Corresponds to Incoloy 800H or Alloy 800H
- UNS N08811: Corresponds to Incoloy 800HT or Alloy 800HT
- UNS N08120: Corresponds to Alloy 801
- UNS N08890: Corresponds to Alloy 890
- Alloy 800, 800H, 800HT